Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen:
Gespeichert in:
1. Verfasser: | |
---|---|
Format: | Buch |
Sprache: | German |
Veröffentlicht: |
1994
|
Schlagworte: | |
Online-Zugang: | Inhaltsverzeichnis |
Beschreibung: | Darmstadt, Techn. Hochsch., Diss., 1993 |
Beschreibung: | XVI, 179 S. Ill., graph. Darst. |
Internformat
MARC
LEADER | 00000nam a2200000 c 4500 | ||
---|---|---|---|
001 | BV009753003 | ||
003 | DE-604 | ||
005 | 19950804 | ||
007 | t | ||
008 | 940803s1994 gw ad|| m||| 00||| ger d | ||
016 | 7 | |a 941432459 |2 DE-101 | |
035 | |a (OCoLC)214471925 | ||
035 | |a (DE-599)BVBBV009753003 | ||
040 | |a DE-604 |b ger |e rakddb | ||
041 | 0 | |a ger | |
044 | |a gw |c DE | ||
049 | |a DE-91 |a DE-12 |a DE-355 |a DE-83 |a DE-11 | ||
084 | |a WER 815d |2 stub | ||
084 | |a WER 830d |2 stub | ||
084 | |a FER 325d |2 stub | ||
084 | |a WER 170d |2 stub | ||
100 | 1 | |a Duchardt, Jürgen |e Verfasser |4 aut | |
245 | 1 | 0 | |a Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen |c vorgelegt von Jürgen Duchardt |
264 | 1 | |c 1994 | |
300 | |a XVI, 179 S. |b Ill., graph. Darst. | ||
336 | |b txt |2 rdacontent | ||
337 | |b n |2 rdamedia | ||
338 | |b nc |2 rdacarrier | ||
500 | |a Darmstadt, Techn. Hochsch., Diss., 1993 | ||
650 | 0 | 7 | |a Martensitumwandlung |0 (DE-588)4131050-0 |2 gnd |9 rswk-swf |
650 | 0 | 7 | |a Austenitischer Stahl |0 (DE-588)4003892-0 |2 gnd |9 rswk-swf |
650 | 0 | 7 | |a Chrom-Nickel-Stahl |0 (DE-588)4132413-4 |2 gnd |9 rswk-swf |
650 | 0 | 7 | |a Tieftemperatur |0 (DE-588)4134801-1 |2 gnd |9 rswk-swf |
650 | 0 | 7 | |a Strecken |0 (DE-588)4344537-8 |2 gnd |9 rswk-swf |
655 | 7 | |0 (DE-588)4113937-9 |a Hochschulschrift |2 gnd-content | |
689 | 0 | 0 | |a Austenitischer Stahl |0 (DE-588)4003892-0 |D s |
689 | 0 | 1 | |a Chrom-Nickel-Stahl |0 (DE-588)4132413-4 |D s |
689 | 0 | 2 | |a Strecken |0 (DE-588)4344537-8 |D s |
689 | 0 | 3 | |a Tieftemperatur |0 (DE-588)4134801-1 |D s |
689 | 0 | 4 | |a Martensitumwandlung |0 (DE-588)4131050-0 |D s |
689 | 0 | |5 DE-604 | |
856 | 4 | 2 | |m DNB Datenaustausch |q application/pdf |u http://bvbr.bib-bvb.de:8991/F?func=service&doc_library=BVB01&local_base=BVB01&doc_number=006450595&sequence=000001&line_number=0001&func_code=DB_RECORDS&service_type=MEDIA |3 Inhaltsverzeichnis |
943 | 1 | |a oai:aleph.bib-bvb.de:BVB01-006450595 |
Datensatz im Suchindex
_version_ | 1812453988501553152 |
---|---|
adam_text |
III
GLIEDERUNG
SEITE
1
.
EINLEITUNG
1
2
.
AUFGABENSTELLUNG
4
3.
3.1
3.2
3.3
3.4
3.5
3.5.1
3.5.2
STAND DES WISSENS
3
VORGAENGE BEI DER KALTVERFORMUNG AUSTENITISCHER 5
STAEHLE
AUSTENITSTABILITAET 6
GEFUEGEUMWANDLUNG UNTER MARTENSITBILDUNG 9
AUSWIRKUNGEN EINER WAERMEBEHANDLUNG AUF DIE MAERTEN- 12
SITISCHE PHASE
AUSWIRKUNGEN DER MARTENSITISCHEN UMWANDLUNG AUF
13
DIE KORROSIONSBESTAENDIGKEIT
VERHALTEN IM AKTIV-PASSIV-BEREICH
LOCHKORROSIONS- UND SPRK-VERHALTEN
14
BIBLIOGRAFISCHE INFORMATIONEN
HTTP://D-NB.INFO/941432459
IV
4
.
4.1
4.2
4.3
4.3.1
HERSTELLUNG KRYOGESTRECKTER WERKSTOFFPROBEN
FUER KORROSIONSVERSUCHE
VERSUCHSWERKSTOFF E
PROBEN AUS EINEM KRYOGESTRECKTEN APPARAT
KRYOSTRECKUNG VON ZUGSTAEBEN IM TECHNIKUM
HERSTELLUNG DER ZUGSTAEBE
4.3.1.1 ALLGEMEINES
4.3.1.2 ZUGSTAEBE AUS 3 MM DICKEM BLECH
4.3.1.3 ZUGSTAEBE AUS 12 MM DICKEM BLECH
4.3.2 DURCHFUEHRUNG DER STRECKUNG AN ZUGSTAEBEN
4.3.3 ABHAENGIGKEIT DER FESTIGKEITSKENNWERTE BEI
RAUMTEMPERATUR VON DER STRECKSPANNUNG BEI
TIEFER TEMPERATUR (KRYOSPANNUNG)
4.3.3.1 ALLGEMEINES
4.3.3.2 ERMITTLUNG DER ABHAENGIGKEIT ZWISCHEN KRYOSPAN
NUNG, KRYODEHNUNG UND DEN FESTIGKEITSKENN
WERTEN BEI RAUMTEMPERATUR
ABHAENGIGKEIT DER CHLORIDBEDINGTEN SPANNUNGS
RISSKORROSION VON VERSCHIEDENEN EINFLUSSGROESSEN
EINFUEHRUNG
SEITE
15
15
18
20
20
20
21
22
23
25
25
25
28
28
5.1
V
5.2 PARAMETER DER CHLORIDBEDINGTEN SPANNUNGSRISS
KORROSION
5.2.1 MEDIUMSEITIGE PARAMETER
5.2.2 WERKSTOFFSEITIGE PARAMETER
6
.
6.1
6
.1.1
6
.
1.2
EXPERIMENTELLES
PROBENFORMEN ZUR UNTERSUCHUNG DER SPRK
FLACHPROBEN MIT KONSTANTER VERFORMUNG
VARIATIONEN DER PROBENBEHANDLUNG
7. AUSSENSTROMLOSE VERSUCHE ZUM SPRK-VERHALTEN VON
FLACHPROBEN IN VOLLENTSALZTEM WASSER MIT EINER
CHLORIDZUGABE VON 100 PPM CI- UND TEMPERATUREN
BIS 200C
V
7.1 ALLGEMEINES
7.2 VERSUCHSWERKSTOFFE
7.3 PROBENHERSTELLUNG UND PROBENGEOMETRIE
7.3.1 KRYOGESTRECKTE PROBEN
7.3.2 PROBEN IM ANLIEFERUNGSZUSTAND
SEITE
29
29
31
35
35
37
38
39
39
40
41
41
42
VI
7.4
7.4.2
7.5
7.5.1
7.5.2
VERSUCHSDURCHFUEHRUNG
7.4.1
VERSUCHE
BEI
TEMPERATUREN
BIS 150 C
VERSUCHE
BEI
TEMPERATUREN
BIS 200* C
VERSUCHSERGEBNISSE
SPRK-VERSUCHE
MIT
UNGESCHLIFFENEN FLACHPROBEN
BEI
TEMPERATUREN
BIS 200C
SPRK
-VERSUCHE MIT GROB GESCHLIFFENEN FLACH-
YYROBEN BEI TEMPERATUREN
BIS 200'C
SEITE
43
43
44
45
45
46
8
.
AUSSENSTROMLOSE
FLACHPROBEN IN
CHLORID-LOESUNG
VERSUCHE ZUM SPRK-VERHALTEN VON
SIEDENDER 42%IGER MAGNESIUM-
ALLGEMEINES
VERSUCHSDURCHFUEHRUNG
8.3
8.3.1
8.3.1.1
8
.
3
.
1.2
8.3.1.3
STAHL DER WNR. 1.4541
IM ANLIEFERUNGSZUSTAND
VER
SUCHSERGEBNISSE
ERGEBNISSE MIT PROBEN AUS
VERHALTEN DES WERKSTOFFES
UNTERSUCHUNGEN ZUM SCHNITTKANTENEFFEKT
I -IN FLUESSIGEM STICKSTOFF
FOLGEN EINER AUSLAGERUNG IN FLUESSIG
48
48
49
51
51
51
51
51
VII
8.
3.1.4
AUSWIRKUNGEN UNTERSCHIEDLICHER KRYOSTRECKUNGEN
8.3.1.5
ABTRAG DURCH BEIZEN UND ELEKTROPOLIEREN NACH DER
KRYOSTRECKUNG
8.
3.1.6
EINFLUSS DES GROBEN SCHLEIFENS IM ANSCHLUSS AN DIE
KRYOSTRECKUNG
8.3.
1.7
WIRKUNG EINER AUSLAGERUNG GROB GESCHLIFFENER
PROBEN IN FLUESSIGEM STICKSTOFF
8.3.1.8 EINFLUSS DES KRYOSTRECKENS AUF GROB GESCHLIFFENE
PROBEN
8.3.
1.9
EINFLUSS EINER BEIZBEHANDLUNG VOR UND NACH DER
KRYOSTRECKUNG EINER GROB UEBERSCHLIFFENEN PROBE
8.3.2
ERGEBNISSE MIT PROBEN AUS STAHL DER WNR.
1.4571
8.3.2.1
VERHALTEN DES WERKSTOFFES IM ANLIEFERUNGSZUSTAND
8.3.2.2 UNTERSUCHUNGEN ZUM SCHNITTKANTENEFFEKT
8 3.2.3
VERHALTEN NACH UNTERSCHIEDLICH HOHEN
KRYO
STRECKUNGEN
8.3.2.4 EINFLUSS DES GROBEN SCHLEIFENS IM ANSCHLUSS AN DIE
KRYOSTRECKUNG
8.3.2.5 WIRKUNG EINER AUSLAGERUNG GROB GESCHLIFFENER
PROBEN IN FLUESSIGEM STICKSTOFF
EINFLUSS DES KRYOSTRECKENS AUF ZUVOR GROB UEBER-
SCHLIFFENE PROBEN
SEITE
52
52
52
53
53
55
56
56
57
57
57
58
8.3.2.6
59
VIII
8.3.2.7 EINFLUSS EINER BEIZBEHANDLUNG VOR UND NACH DER
KRYOSTRECKUNG EINER GROB UEBERSCHLIFFENEN PROBE
8.3.3 ZUSAMMENFASSUNG DER ERGEBNISSE AUSSENSTROMLOSER
VERSUCHE MIT FLACHPROBEN AUS STAHL DER WNM.
1.4541 UND 1.4571 IN SIEDENDER 42%IGER MGC12-
LOESUNG
SEITE
60
61
9.
9.1
9.2
AUSSENSTROMLOSE VERSUCHE ZUM SPRK-VERHALTEN
VON RUNDZUGPROBEN UNTER KONSTANTER LAST IN SIE
DENDER 42%IGER MAGNESIUMCHLORIDLOESUNG
ALLGEMEINES
HERSTELLUNG VON RUNDZUGPROBEN MIT GLATTER PRUEF
STRECKE
62
62
63
9.3
9.4
VERSUCHSDURCHFUEHRUNG
VERSUCHSERGEBNIS SE
9.4.1 UNGESTRECKTE PROBEN AUS STAHL DER WNR. 1.4541,
NICHT ELEKTROPOLIERT
9.4.2 UNGESTRECKTE PROBEN AUS STAHL DER WNR. 1.4541,
ELEKTROPOLIERT
9.4.3 UNGESTRECKTE PROBEN AUS STAHL DER WNR. 1.4541,
GEGLUEHT UND ELEKTROPOLIERT
64
65
65
66
67
9.4.4 KRYOGESTRECKTE PROBEN AUS STAHL DER WNR. 1.4541,
NICHT ELEKTROPOLIERT
68
IX
SEITE
9.4.5 KRYOGESTRECKTE PROBEN AUS STAHL DER WNR. 1.4541, 69
ELEKTROPOLIERT
9.4.6 FOLGERUNGEN FUER DIE PRAKTISCHE ANWENDUNG 69
9.4.7 PROBEN AUS STAHL DER WNR. 1.4571, ELEKTRO- 71
POLIERT
10. AUSSENSTROMLOSE VERSUCHE ZUM SPRK-VERHALTEN 72
VON KLEINAPPARATEN UND ROHREN IN SIEDENDER
42%IGER MAGNESIUMCHLORIDLOESUNG
10.1 ALLGEMEINES 72
10.2 HERSTELLUNG DER VERSUCHSKOERPER 72
10.3 KRYOSTRECKUNG DER VERSUCHSKOERPER 73
10.4 VERSUCHSDURCHFUEHRUNG 75
10.5 ERGEBNISSE DER EINZELVERSUCHE 76
10.6 , ZUSAMMENFASSUNG DER ERGEBNISSE 79
11. POTENTIALKONTROLLIERTE VERSUCHE IN VOLLENT- 80
SALZTEM WASSER MIT EINER CHLORIDZUGABE VON
100 PPM CI- UND VERSCHIEDENEN TEMPERATUREN
11.1 ALLGEMEINES 80
X
SEITE
11.2 VERSUCHSWERKSTOFFE 81
11.3 PROBENHERSTELLUNG UND PROBENGEOMETRIE 81
11.4 VERSUCHSDURCHFUEHRUNG 82
11.5 VERSUCHSERGEBNISSE 83
11.5.1 PROBEN AUS STAHL DER WNR. 1.4541 83
11.5.2 PROBEN AUS STAHL DER WNR. 1.4571 84
12. UNTERSUCHUNG DER BESTAENDIGKEIT GEGEN LOCH- 85
KORROSION
12.1 EINFUEHRUNG 85
12.2 PARAMETER DER LOCHKORROSION 87
12.2.1 MEDIUMSEITIGE PARAMETER 87
*
12.2.2 WERKSTOFFSEITIGE PARAMETER 89
12.3 EXPERIMENTELLES 90
12.3.1 VERSUCHSGRUNDLAGEN 90
12.3.2 VERSUCHSWERKSTOFFE 91
12.3.3 PROBENVORBEHANDLUNG 92
12.3.4 VERSUCHSDURCHFUEHRUNG 92
XI
SEITE
12.4 ERGEBNISSE DER UNTERSUCHUNGEN ZUR BESTAENDIG- 94
KEIT GEGEN LOCHKORROSION
13. ANALYTISCHE BESTIMMUNG VON EIGENSPANNUNGEN 95
UND WERKSTOFFPHASEN MITTELS ROENTGENFEIN
STRUKTURUNTERSUCHUNG
13.1 EINFUEHRUNG
95
13.2 EIGENSPANNUNGEN
98
13.3 MESSUNG DER EIGENSPANNUNGEN MITTELS ROENTGEN- 100
FEINSTRUKTURANALYSE
13.4 BESTIMMUNG DES RESTAUSTENITGEHALTES MITTELS 101
ROENTGENFEINSTRUKTURANALYSE
13.5 DURCHFUEHRUNG DER UNTERSUCHUNGEN 102
13.5.1 PHASENANALYSEN 102
13.5.2 EIGENSPANNUNGSMESSUNGEN 103
13.5.3 ERGEBNISSE DER PHASEN- UND EIGENSPANNUNGS- 103
ANALYSEN
13.6 EINFLUSS DER AUSTENIT- MARTENSIT- UMWANDLUNG 105
AUF DEN EIGENSPANNUNGSZUSTAND UND DAS SPRK-
VERHALTEN
13.6.1 LOESUNGSGEGLUEHTE PROBEN, KRYOGESTRECKT 105
XII
13.6.2 KRYOGESTRECKTE RUNDZUGPROBEN UNTER KON
STANTER BELASTUNG
13.6.3 GROB GESCHLIFFENE FLACHPROBEN
13.6.3.1 GROB GESCHLIFFENE FLACHPROBEN, KRYOGESTRECKT
13.6.3.2 KRYOGESTRECKTE FLACHPROBEN, GROB GESCHLIFFEN
SEITE
106
107
107
110
14.
EIGNUNG NICHTROSTENDER AUSTENITISCHER STAEHLE
FUER DIE PRAKTISCHE ANWENDUNG DES KRYOSTRECKENS
111
15.
ZUSAMMENFASSUNG
113
16.
LITERATURVERZEICHNIS
117
17.
TABELLEN UND BILDER
122 |
any_adam_object | 1 |
author | Duchardt, Jürgen |
author_facet | Duchardt, Jürgen |
author_role | aut |
author_sort | Duchardt, Jürgen |
author_variant | j d jd |
building | Verbundindex |
bvnumber | BV009753003 |
classification_tum | WER 815d WER 830d FER 325d WER 170d |
ctrlnum | (OCoLC)214471925 (DE-599)BVBBV009753003 |
discipline | Werkstoffwissenschaften Fertigungstechnik |
format | Book |
fullrecord | <?xml version="1.0" encoding="UTF-8"?><collection xmlns="http://www.loc.gov/MARC21/slim"><record><leader>00000nam a2200000 c 4500</leader><controlfield tag="001">BV009753003</controlfield><controlfield tag="003">DE-604</controlfield><controlfield tag="005">19950804</controlfield><controlfield tag="007">t</controlfield><controlfield tag="008">940803s1994 gw ad|| m||| 00||| ger d</controlfield><datafield tag="016" ind1="7" ind2=" "><subfield code="a">941432459</subfield><subfield code="2">DE-101</subfield></datafield><datafield tag="035" ind1=" " ind2=" "><subfield code="a">(OCoLC)214471925</subfield></datafield><datafield tag="035" ind1=" " ind2=" "><subfield code="a">(DE-599)BVBBV009753003</subfield></datafield><datafield tag="040" ind1=" " ind2=" "><subfield code="a">DE-604</subfield><subfield code="b">ger</subfield><subfield code="e">rakddb</subfield></datafield><datafield tag="041" ind1="0" ind2=" "><subfield code="a">ger</subfield></datafield><datafield tag="044" ind1=" " ind2=" "><subfield code="a">gw</subfield><subfield code="c">DE</subfield></datafield><datafield tag="049" ind1=" " ind2=" "><subfield code="a">DE-91</subfield><subfield code="a">DE-12</subfield><subfield code="a">DE-355</subfield><subfield code="a">DE-83</subfield><subfield code="a">DE-11</subfield></datafield><datafield tag="084" ind1=" " ind2=" "><subfield code="a">WER 815d</subfield><subfield code="2">stub</subfield></datafield><datafield tag="084" ind1=" " ind2=" "><subfield code="a">WER 830d</subfield><subfield code="2">stub</subfield></datafield><datafield tag="084" ind1=" " ind2=" "><subfield code="a">FER 325d</subfield><subfield code="2">stub</subfield></datafield><datafield tag="084" ind1=" " ind2=" "><subfield code="a">WER 170d</subfield><subfield code="2">stub</subfield></datafield><datafield tag="100" ind1="1" ind2=" "><subfield code="a">Duchardt, Jürgen</subfield><subfield code="e">Verfasser</subfield><subfield code="4">aut</subfield></datafield><datafield tag="245" ind1="1" ind2="0"><subfield code="a">Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen</subfield><subfield code="c">vorgelegt von Jürgen Duchardt</subfield></datafield><datafield tag="264" ind1=" " ind2="1"><subfield code="c">1994</subfield></datafield><datafield tag="300" ind1=" " ind2=" "><subfield code="a">XVI, 179 S.</subfield><subfield code="b">Ill., graph. Darst.</subfield></datafield><datafield tag="336" ind1=" " ind2=" "><subfield code="b">txt</subfield><subfield code="2">rdacontent</subfield></datafield><datafield tag="337" ind1=" " ind2=" "><subfield code="b">n</subfield><subfield code="2">rdamedia</subfield></datafield><datafield tag="338" ind1=" " ind2=" "><subfield code="b">nc</subfield><subfield code="2">rdacarrier</subfield></datafield><datafield tag="500" ind1=" " ind2=" "><subfield code="a">Darmstadt, Techn. Hochsch., Diss., 1993</subfield></datafield><datafield tag="650" ind1="0" ind2="7"><subfield code="a">Martensitumwandlung</subfield><subfield code="0">(DE-588)4131050-0</subfield><subfield code="2">gnd</subfield><subfield code="9">rswk-swf</subfield></datafield><datafield tag="650" ind1="0" ind2="7"><subfield code="a">Austenitischer Stahl</subfield><subfield code="0">(DE-588)4003892-0</subfield><subfield code="2">gnd</subfield><subfield code="9">rswk-swf</subfield></datafield><datafield tag="650" ind1="0" ind2="7"><subfield code="a">Chrom-Nickel-Stahl</subfield><subfield code="0">(DE-588)4132413-4</subfield><subfield code="2">gnd</subfield><subfield code="9">rswk-swf</subfield></datafield><datafield tag="650" ind1="0" ind2="7"><subfield code="a">Tieftemperatur</subfield><subfield code="0">(DE-588)4134801-1</subfield><subfield code="2">gnd</subfield><subfield code="9">rswk-swf</subfield></datafield><datafield tag="650" ind1="0" ind2="7"><subfield code="a">Strecken</subfield><subfield code="0">(DE-588)4344537-8</subfield><subfield code="2">gnd</subfield><subfield code="9">rswk-swf</subfield></datafield><datafield tag="655" ind1=" " ind2="7"><subfield code="0">(DE-588)4113937-9</subfield><subfield code="a">Hochschulschrift</subfield><subfield code="2">gnd-content</subfield></datafield><datafield tag="689" ind1="0" ind2="0"><subfield code="a">Austenitischer Stahl</subfield><subfield code="0">(DE-588)4003892-0</subfield><subfield code="D">s</subfield></datafield><datafield tag="689" ind1="0" ind2="1"><subfield code="a">Chrom-Nickel-Stahl</subfield><subfield code="0">(DE-588)4132413-4</subfield><subfield code="D">s</subfield></datafield><datafield tag="689" ind1="0" ind2="2"><subfield code="a">Strecken</subfield><subfield code="0">(DE-588)4344537-8</subfield><subfield code="D">s</subfield></datafield><datafield tag="689" ind1="0" ind2="3"><subfield code="a">Tieftemperatur</subfield><subfield code="0">(DE-588)4134801-1</subfield><subfield code="D">s</subfield></datafield><datafield tag="689" ind1="0" ind2="4"><subfield code="a">Martensitumwandlung</subfield><subfield code="0">(DE-588)4131050-0</subfield><subfield code="D">s</subfield></datafield><datafield tag="689" ind1="0" ind2=" "><subfield code="5">DE-604</subfield></datafield><datafield tag="856" ind1="4" ind2="2"><subfield code="m">DNB Datenaustausch</subfield><subfield code="q">application/pdf</subfield><subfield code="u">http://bvbr.bib-bvb.de:8991/F?func=service&doc_library=BVB01&local_base=BVB01&doc_number=006450595&sequence=000001&line_number=0001&func_code=DB_RECORDS&service_type=MEDIA</subfield><subfield code="3">Inhaltsverzeichnis</subfield></datafield><datafield tag="943" ind1="1" ind2=" "><subfield code="a">oai:aleph.bib-bvb.de:BVB01-006450595</subfield></datafield></record></collection> |
genre | (DE-588)4113937-9 Hochschulschrift gnd-content |
genre_facet | Hochschulschrift |
id | DE-604.BV009753003 |
illustrated | Illustrated |
indexdate | 2024-10-09T16:20:16Z |
institution | BVB |
language | German |
oai_aleph_id | oai:aleph.bib-bvb.de:BVB01-006450595 |
oclc_num | 214471925 |
open_access_boolean | |
owner | DE-91 DE-BY-TUM DE-12 DE-355 DE-BY-UBR DE-83 DE-11 |
owner_facet | DE-91 DE-BY-TUM DE-12 DE-355 DE-BY-UBR DE-83 DE-11 |
physical | XVI, 179 S. Ill., graph. Darst. |
publishDate | 1994 |
publishDateSearch | 1994 |
publishDateSort | 1994 |
record_format | marc |
spelling | Duchardt, Jürgen Verfasser aut Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen vorgelegt von Jürgen Duchardt 1994 XVI, 179 S. Ill., graph. Darst. txt rdacontent n rdamedia nc rdacarrier Darmstadt, Techn. Hochsch., Diss., 1993 Martensitumwandlung (DE-588)4131050-0 gnd rswk-swf Austenitischer Stahl (DE-588)4003892-0 gnd rswk-swf Chrom-Nickel-Stahl (DE-588)4132413-4 gnd rswk-swf Tieftemperatur (DE-588)4134801-1 gnd rswk-swf Strecken (DE-588)4344537-8 gnd rswk-swf (DE-588)4113937-9 Hochschulschrift gnd-content Austenitischer Stahl (DE-588)4003892-0 s Chrom-Nickel-Stahl (DE-588)4132413-4 s Strecken (DE-588)4344537-8 s Tieftemperatur (DE-588)4134801-1 s Martensitumwandlung (DE-588)4131050-0 s DE-604 DNB Datenaustausch application/pdf http://bvbr.bib-bvb.de:8991/F?func=service&doc_library=BVB01&local_base=BVB01&doc_number=006450595&sequence=000001&line_number=0001&func_code=DB_RECORDS&service_type=MEDIA Inhaltsverzeichnis |
spellingShingle | Duchardt, Jürgen Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen Martensitumwandlung (DE-588)4131050-0 gnd Austenitischer Stahl (DE-588)4003892-0 gnd Chrom-Nickel-Stahl (DE-588)4132413-4 gnd Tieftemperatur (DE-588)4134801-1 gnd Strecken (DE-588)4344537-8 gnd |
subject_GND | (DE-588)4131050-0 (DE-588)4003892-0 (DE-588)4132413-4 (DE-588)4134801-1 (DE-588)4344537-8 (DE-588)4113937-9 |
title | Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen |
title_auth | Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen |
title_exact_search | Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen |
title_full | Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen vorgelegt von Jürgen Duchardt |
title_fullStr | Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen vorgelegt von Jürgen Duchardt |
title_full_unstemmed | Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen vorgelegt von Jürgen Duchardt |
title_short | Zum Verhalten kryogestreckter austen[i]tischer Stähle gegen Spannungsrisskorrosion und Lochkorrosion unter praxisnahen Bedingungen |
title_sort | zum verhalten kryogestreckter austen i tischer stahle gegen spannungsrisskorrosion und lochkorrosion unter praxisnahen bedingungen |
topic | Martensitumwandlung (DE-588)4131050-0 gnd Austenitischer Stahl (DE-588)4003892-0 gnd Chrom-Nickel-Stahl (DE-588)4132413-4 gnd Tieftemperatur (DE-588)4134801-1 gnd Strecken (DE-588)4344537-8 gnd |
topic_facet | Martensitumwandlung Austenitischer Stahl Chrom-Nickel-Stahl Tieftemperatur Strecken Hochschulschrift |
url | http://bvbr.bib-bvb.de:8991/F?func=service&doc_library=BVB01&local_base=BVB01&doc_number=006450595&sequence=000001&line_number=0001&func_code=DB_RECORDS&service_type=MEDIA |
work_keys_str_mv | AT duchardtjurgen zumverhaltenkryogestreckteraustenitischerstahlegegenspannungsrisskorrosionundlochkorrosionunterpraxisnahenbedingungen |